| Chromemoly Tubing - suggestions |
|
General
|
- This is a self-annealing weld.
|
|
Torch Tip
|
- use the #00 for 26 to 28 ga.
- use the #0 for 24 to 20 ga
- use the #0.5 for 18 to 20ga
- use the #1 for 16 to 1/8"
- use the #2 for 1/8" and thicker
- the #2.5 tip may be helpfull on 3/8" and thicker
|
|
Gas Settings
|
- use 4 to 4 1/2 psi on both gases
- if a 50' hose is used, increase your pressure 1 to 2 psi (see
setting up the torch)
|
|
Flame Setting
|
- Use a neutral or just off feather
- See setting up torch
|
|
Flux
|
- no flux required or recommended for chromemoly.
|
|
Rod Selection
|
Rod material
- We recommend the ER70S-2 (TIG) or oxweld #32
When sizing your rod
- 1/16" for 0.030.
- 3/32" for thicker
|
|
Technique
|
- Move torch in slow small increments - wide oscillations are
not necessary.
- Do not remove flame from metal abruptly as this may crystallize
the weld.
|